Bitumen Grade Equivalence Chart — Penetration, VG, PG, AC and Australian Grades Compared

Bitumen grade equivalence chart - penetration, viscosity and performance grade comparison

There is no exact bitumen grade equivalence between grading systems, and any chart that claims otherwise is misleading you. Penetration, viscosity, performance and AC grading each measure different properties at different temperatures. What this guide gives you is the practical cross-reference used in trade — which grade is typically supplied against which specification — along with a clear explanation of where the equivalence breaks down and why that matters on a tender.

Systems coveredPenetration · VG · PG · AC · Australian
StandardsEN 12591 · IS 73 · AASHTO M320 · ASTM D3381 · AS 2008
Grades suppliedAll families, single or mixed shipment
Minimum order100 MT
Loading portsJebel Ali · Mersin · Bandar Abbas
CertificationBatch COA against the named standard
InspectionSGS / Bureau Veritas on request
TermsFOB / CFR / CIF

Why exact bitumen grade equivalence does not exist

This is the part most conversion charts leave out, and it is the reason a substitution that looks safe on paper can fail a tender.

Each grading system measures a different property, at a different temperature, on a differently conditioned sample:

System What it measures At what temperature Sample condition
Penetration Depth a standard needle sinks in 5 seconds 25 °C Original binder
Viscosity (VG) Absolute viscosity, resistance to flow 60 °C Original binder
Performance (PG) Rheology across the full service range Multiple, from −22 to +76 °C Original, RTFO-aged and PAV-aged
AC Absolute viscosity in poise 60 °C Original binder
Australian (C) Viscosity in pascal-seconds 60 °C Original binder

Two binders can match on one test and diverge on another. Two products both meeting 60/70 at 25 °C can behave quite differently at 60 °C, because penetration says nothing about temperature susceptibility. That is precisely the gap viscosity grading was introduced to close, and the gap PG grading closes further by testing after simulated ageing.

So use the tables below as a sourcing guide, not a specification substitution. If your contract names a grade, the certificate must state that grade tested to that standard.

Bitumen grade equivalence: penetration to viscosity grade

The most frequently requested cross-reference, because penetration grading dominates Europe, the Middle East and Africa while viscosity grading dominates India and much of South Asia.

Penetration grade Pen @25 °C (dmm) Typical VG match Viscosity @60 °C Common use
80/100 80–100 VG10 800–1200 poise Spray work, prime and tack coats, low-traffic roads
70/100 70–100 VG20 1600–2400 poise Moderate traffic, cooler climates
60/70 60–70 VG30 2400–3600 poise The global default for highways and urban roads
40/50 40–50 VG40 3200–4800 poise Hot climates, airport pavements, heavy slow loading
30/40 30–40 Above VG40 Not classified Extreme heat, industrial hardstanding

VG grades are defined in IS 73; penetration grades in EN 12591 and ASTM D946. A binder meeting 60/70 will not automatically pass VG30 — the correlation is typical, not guaranteed.

Bitumen grade equivalence: penetration to AC grade

AC grading, defined in ASTM D3381, is the older American viscosity system. It still appears in specifications across Latin America, parts of the Middle East and legacy contracts.

AC grade Viscosity @60 °C Typical penetration match Typical VG match
AC-10 1000 ±200 poise 80/100 VG10
AC-20 2000 ±400 poise 60/70 VG20 to VG30
AC-30 3000 ±600 poise 50/70 VG30
AC-40 4000 ±800 poise 40/50 VG40

The AC number is the target viscosity in hundreds of poise. AC-20 and VG20 are not the same — they use different tolerance bands and, in some cases, different test conditioning. See our AC bitumen page for the full specification.

Bitumen grade equivalence: penetration to performance grade

PG grading works differently from everything above, and treating it as another viscosity scale is the single most common error we see on tender documents.

PG numbers are pavement design temperatures, not binder properties. In PG 64-22, the 64 is the seven-day average maximum pavement temperature the binder must resist in degrees Celsius, and the −22 is the minimum pavement temperature it must survive. The binder is tested at both extremes, and after simulated short-term and long-term ageing.

PG grade Design temperature range Typical penetration match Modified? Where it is specified
PG 58-16 +58 to −16 °C 80/100 No Temperate climates, moderate traffic
PG 64-22 +64 to −22 °C 60/70 No The most widely used PG grade worldwide
PG 70-10 +70 to −10 °C 40/50 to 60/70 Usually not Hot climates without severe winters — Gulf, North Africa
PG 70-16 +70 to −16 °C 40/50 Sometimes Hot climates, heavy traffic corridors
PG 76-10 +76 to −10 °C Modified base Yes Extreme heat, port aprons, intersections
PG 76-16 +76 to −16 °C Modified base Yes Airport pavements, heavy industrial loading
PG 76-22 +76 to −22 °C Modified base Yes Wide temperature range with heavy traffic

The useful temperature interval rule

Add the two PG numbers together, ignoring the sign, and you get the useful temperature interval. PG 64-22 has an interval of 86 degrees. PG 76-22 has 98.

An unmodified binder can generally achieve up to roughly 90 degrees of interval straight from refining. Above that, polymer modification is required. That single calculation tells you whether a PG grade in a tender will need PMB or whether a straight refinery product will meet it — useful before you price the job.

Bitumen grade equivalence: Australian C grades

Australian grading under AS 2008 uses viscosity in pascal-seconds at 60 °C. The grade number is the target viscosity value.

Australian grade Viscosity @60 °C Typical penetration match Typical use
C170 140–200 Pa·s 80/100 Spray sealing, general sealing work
C240 200–280 Pa·s 60/70 to 70/100 Asphalt production, moderate traffic
C320 260–380 Pa·s 60/70 The most widely used Australian paving grade
C450 370–530 Pa·s 40/50 Heavy duty asphalt, high traffic
C600 500–700 Pa·s 30/40 to 40/50 Extreme loading, industrial pavement

Full specifications on our Australian grade bitumen page.

Which grading system is used where

Knowing which system a market works in tells you what a buyer’s tender will name before they send it.

Region Dominant system Standard Notes
Europe, Middle East, most of Africa Penetration EN 12591 / ASTM D946 60/70 is the default across most of the region
India, Bangladesh, Nepal, parts of Africa Viscosity (VG) IS 73 Also appears wherever Indian contractors work
United States, Canada Performance (PG) AASHTO M320 Superpave system, now the North American norm
Latin America, legacy contracts AC and penetration ASTM D3381 PG increasingly specified on newer work
Australia, New Zealand Class (C) AS 2008 Separate multigrade and PMB classes exist
South Africa Penetration SANS 4001-BT1 Modified binders under SATS 3208 on high-traffic work

How to use a bitumen grade equivalence chart safely

Four rules, in order of how much money they save.

1. The certificate must match the specification, not the equivalence. If a tender names VG30, a certificate showing 60/70 to EN 12591 does not satisfy it, however close the material is. Ask your supplier to certify against the named standard.

2. Equivalence works better within a system than across it. Moving between two penetration grades is predictable. Moving from a penetration grade to a PG grade is not, because PG tests properties that penetration grading never measures.

3. Check the ageing requirement. PG grading tests after RTFO and PAV conditioning. Penetration and viscosity grading generally do not. A binder can meet 60/70 comfortably and still fail PG 64-22 on the low-temperature BBR test.

4. When in doubt, send the specification rather than the grade name. A supplier who can read a tender specification will tell you what actually meets it. One who only recognises grade names will guess.

Grades outside the paving systems

Two families are graded on entirely different principles and have no equivalence to the tables above.

Oxidized bitumen is named by softening point and penetration together — 85/25 means a softening point around 85 °C and penetration of 20 to 30 dmm. It is a waterproofing and industrial material, not a paving binder, and cannot substitute for any penetration grade.

Cutback and emulsion grades are named by curing or setting speed — MC-70, RC-250, CSS-1h. These are application products carrying a base binder, not binder grades in themselves. See our comparison of cutback bitumen vs bitumen emulsion.

Frequently asked questions about bitumen grade equivalence

These are the questions we are asked most often when a buyer is working across two grading systems.

What is the VG30 equivalent in penetration grade?

60/70 is the typical match. VG30 has an absolute viscosity of 2400 to 3600 poise at 60 °C under IS 73; 60/70 has a penetration of 60 to 70 dmm at 25 °C. They usually correspond in practice, but the tests measure different properties and a binder meeting one does not automatically pass the other.

Is PG 64-22 the same as 60/70?

Typically comparable but not the same. PG 64-22 describes pavement design temperatures and is verified across the full service range after simulated ageing; 60/70 describes consistency at a single temperature of 25 °C on unaged binder. Most PG 64-22 material falls in the 60/70 penetration band, but the reverse does not hold — plenty of 60/70 binders would fail the PG 64-22 low-temperature requirement.

What is AC-20 equivalent to?

Roughly 60/70 penetration grade, or VG20 to VG30 depending on the exact viscosity. AC-20 targets 2000 poise at 60 °C with a tolerance of plus or minus 400. Note that AC and VG grades with the same number are not interchangeable — the tolerance bands and conditioning differ.

Which Australian grade matches 60/70?

C320 in most cases, and C240 where the specification allows a softer binder. C320 is the most widely used Australian paving grade and typically corresponds to 60/70 penetration material.

Can I substitute one grade for another if the chart says they match?

Not without approval from the specifying engineer. An equivalence chart tells you what is typically supplied against a specification; it does not tell you what will pass an audit. If the contract names a grade and standard, the certificate of analysis must show that grade tested to that standard.

How do I know if a PG grade needs polymer modification?

Add the two numbers, ignoring the sign, to get the useful temperature interval. PG 64-22 gives 86 degrees, which an unmodified refinery binder can generally achieve. Above roughly 90 degrees — PG 76-22 at 98, for example — polymer modification is required. That calculation tells you the cost implication before you price the job.

Does oxidized bitumen have a penetration grade equivalent?

No. Oxidized grades are named by softening point and penetration together, and they are produced by air blowing rather than straight distillation. They are waterproofing and industrial materials with a much higher softening point than any paving binder, and they cannot substitute for a penetration grade in a pavement.

Can you supply against any of these grading systems?

Yes. We ship penetration grades to EN 12591 and ASTM D946, viscosity grades to IS 73, performance grades to AASHTO M320, AC grades to ASTM D3381 and Australian class grades to AS 2008, with a batch certificate of analysis stating the standard tested against. Mixed grades in one shipment are accepted provided each grade reaches one full container.

Reference standards

The specifications behind each system are published by the bodies below. Where a tender cites a clause number, it will come from one of these.

Not sure which grade your specification requires?

Send us the tender specification rather than the grade name. We will confirm what meets it, tell you whether polymer modification is required, and issue a batch certificate of analysis against the standard your contract names. If two grades would both work and one is cheaper, we will say which.

Dubai +971 4 566 4998 · Ankara +90 507 246 9520 · Isfahan +98 31 3235 5207